1、纸箱测试报告纸箱测试报告The test reportThe sample informationThe sample name: cartonSample number: 1-5Sample models: 100 * 100 mlSample type: ABSample size: 479 * 247 * 280 mmSample quantity: 5Sample: normalThe test information Test project: inside diameter, outside diameter, shake cover aperture, shake cover d
2、islocation, the thickness of the cardboard, cardboard g, shake cover folding, marginal pressure strength, burst strength, compression chamber, water content, the printing is wiped, connection strengthReceived date: 2015-08-30The test date: 2016-03-10Test environment (23 + / - 1) , (50 + 2) % RHFigur
3、e 1 corrugated carton sample figureTesting project 1: inner diameter, outside diameter1. The test standard: no2. Test equipment: standard steel ruler3. Test method:3.1 hold up for measurement of the carton, the bottom shake cover fold into the inside, on a flat, smooth surface is measured.3.2 measur
4、ing inner diameter length between the plate on both sides of the box, steel ruler as far as possible will be tight length direction on both sides of the carton board, first in the side of the carton board fixed steel ruler, zero it stretch to the other side of the plate, keep parallel with carton bo
5、ard, read the measurement results.Measuring inner diameter 3.3 on both sides of the box in the width direction board width size, feet as far as possible will be tight width on both sides of the carton board, as previously described step width measurement results.3.4 shake on both ends of the cover f
6、olded, measuring inner diameter height of the carton between roll cover on both ends. When measuring the foot against the wall, at the bottom of the roll cover fixed ruler, zero along the case board straight feet first cover the roots, keep the feet close to the chest wall, keep the vertical positio
7、n accurately, read the measurement results.3.5 outside diameter measurement in the ASTM standard, there is no detailed description, referring to the measurement of inner diameter, first fixed steel ruler zero at one end, then extended to the other measurements.4. The test details:4.1 the testing pro
8、cess: (1) sampling to test samples provided by the company folded neatly, temporarily not top and bottom rock cover seal.(2) test: according to the above test method shows the steps in the measured the cartons inside diameter size of length, width and height, length, width and height and then measur
9、ing diameter size.4.2 the test dataMeasurement data is accurate to 1 mm, each direction should be mobile position measuring at least five sets of data, records in the table.(a) (b) (c)FIG. 1-1 diameter test photos Table 1-1 diameter test results unit:mm timesItems 12345average valuelength468.1468.14
10、70.2469.1471.1469.3wide237.1238.2237.2238.1237.0237.5high263.1262.0263.0262.1262.2262.5(a) (b) (c)Figure 1-2 diameter test photos Table 1-2 diameter test results unit:mm timesitems12345average valuelength483.1482.0484.0484.0484.0483.4wide246.1244.0246.1248.0247.0246.2high269.1270.1269.2268.0268.0268
11、.9Test item 2: shake cover the gap1. The test standard: no2. Test equipment: steel ruler3. Test method:Gaps in the middle cover gap for wave after the cover can be folded in half, folding cartons after molding, with the hand gently close the lid, with accuracy of 1 mm steel ruler to measure the gaps
12、 in the middle bottom and top five groups each, and averaged.4. The test details:4.1 the testing process (1) sampling: hold up the carton samples, top and bottom cover closed gently, do not take the external medium sealing.(2) test: will provide the carton samples hold up, with the hand gently close
13、d the bottom cover, placed on a flat, smooth the surface of the table, and then gently close the upper cover, carton, light pressure measuring upper folded after two roll cover in the middle of the distance. Then gently close the upper part of the wave inversion, ditto shakes the gaps between the co
14、ver at the bottom of the distance measurement.4.2 the test dataPrecise measurement results to 1 mm, top and bottom rock cover clearance of at least five sets of data, average. (a) (b)Figure 2 shake cover aperture test photosTable 2 shake cover aperture test resultsunit:mm timesitems12345average valu
15、eAt the top of the0.51.02.01.51.21.2At the bottom of the2.01.51.00.50.51.1Test project 3: shake cover dislocation1. The test standard: no2. Test equipment: steel ruler3. Test method: cover dislocation is wave cover can be folded in half, both sides shook at the ends of the cover length direction dis
16、placement distance. After molding, folding cartons, with the hand gently closed the cover, shake cover can be folded in half closed, measured with a precision of 1 mm steel rule shake misplaced after cover closed.4. The test details: 4.1 the testing process(1) sampling: hold up the carton samples, t
17、op and bottom cover closed gently, do not take the external medium sealing.(2) test: will provide the carton samples hold up, with the hand gently closed the bottom cover, placed on a flat, smooth the surface of the table, and then gently close the upper cover, carton, light pressure measurement can
18、 be folded in half after the upper two roll cover length direction of dislocation distance. Then gently close the upper part of the wave inversion, ditto distance measuring misalignment of the bottom two roll cover length direction.4.2 the test dataPrecise measurement results to 1 mm, top and bottom
19、 rock cover dislocation distance at least every five sets of data. (a) (b)图3摇盖错位测试照片表3摇盖错位测试结果unit:mm timesitems12345average valueAt the top of the4.05.03.04.03.03.8At the bottom of the3.04.55.05.05.04.5Test item 4: the thickness of the cardboard1. The test standard: ASTM D6452. Test equipment:Devic
20、e nameunit typeequipment numberThe period of validity of calibrationThe table pointer type thickness gaugeGT-313-A- Adjustable paper cutting knives-3. Test method:3.1 before the test on the micrometer thickness gauge calibration, guarantee the presser foot and chopping block besmirch, instrument to
21、place in a fixed table, prevent the happening of the vibration.3.2 the location of the sample placed on the chopping block, to be able to guarantee a point on the edge of the contact surface of at least 6 mm above the sample edge distance.3.3 in all cases, each sample measured at least five times.3.
22、4 at the end of the stop in time to read the data, if necessary, the results with the deviation when the calibration.3.5 presser foot drop rate and to stop in time within the prescribed scope, side paperboard compression makes the measurement is not accurate. 50 + 2 kpa pressure of foot, to stop in
23、time for 3 + 1 s, presser foot drop speed was 0.8 + / - 0.1 mm/s.4. The test details:4.1 the testing process(1) sampling: cardboard sample to box board, box board around corners and center sampling, for a total of five samples, size is 100 mm * 100 mm.(2) test: first of all to calibration of instrum
24、ents, adjust the instrument zero, place the sample between the measured surface, to be able to guarantee a point on the edge of the contact surface of at least 6 mm above the sample edge distance. Test slowly at a rate of 0.8 + / - 0.1 mm/s will be another measure on face gently moved to sample, pay
25、 attention to avoid any impact, after being indicated value stability, before the board is sag, usually finish reading in 2-4 s.4.2 the test dataMeasurements in mm, read the data on the micrometer, accurate to one decimal places, record five sample measured results.Figure 4 board thickness test phot
26、osTable 4 board thickness test tableunit:mm timesitems12345average value17.957.947.927.977.907.9427.978.068.018.018.048.0237.927.917.927.917.957.9247.407.387.507.497.357.4257.787.757.787.767.797.77overall mean7.81Testing project 5: cardboard g1. The test standard: ASTM D646-1996 (2001).2. Test equip
27、ment:Device nameunit typeequipment numberThe period of validity of calibrationelectronic scalesAB204-N- electronic scales-3. Test method:3.1 when use scales to avoid air flow.3.2 humidity had a great influence on the measured value of the paper gram, before the test sample must be in the constant te
28、mperature and humidity test chamber processing more than 24 hours.4. The test details:4.1 the testing process: (1) sampling board sample box board, box board around corners and center part of the sampling, a total of samples from 10, size is 100 mm * 100 mm.(2) test: the laboratory of electronic pre
29、cision balance, measured 10 the quality of the sample piece, accurate to three decimal places.4.2 the test dataAccording to the formula to calculate G, G the cardboard G, M for the quality of the electronic precision measurement scales. For ten sample take arithmetic average, can have to average gra
30、m weight of the cartons.Figure 5 cardboard g test photosTable 5 cardboard g test table timesitemsThe electronic balance reading(g)Cardboard g(g/m2)112.92131292.1212.89181289.2312.86111286.1413.01761301.8512.97911297.9613.01101301.1713.02781302.8813.01041301.0913.04441304.41012.82181282.2mean1295.9 Test item 6: shake cover folding1. The test standard: no2. Test equipment: no3. Test method:According to the test requirements, the shake cover folding test using artificial fold test, does not involve folding test machine.4. The te